ZHAO Jinguo*,QIAO Xun,YAN Zhian.Effect of Heat Treatment on Hardness and Self-Lubrication of Ni-P-BN(h) Composite Coating[J].Plating & Finishing,2022,(1):63-68.[doi:10.3969/j.issn.1001-3849.2022.01.011]
热处理对Ni-P-BN(h)镀层硬度和自润滑性能的影响
- Title:
- Effect of Heat Treatment on Hardness and Self-Lubrication of Ni-P-BN(h) Composite Coating
- 关键词:
- 化学共沉积; Ni-P-BN(h); 热处理; 复合镀层; 自润滑性能
- 分类号:
- TG166
- 文献标志码:
- A
- 摘要:
- 本文对Q235钢表面先后实施化学共沉积和热处理形成Ni-P-BN(h)复合镀层,利用电子探针显微分析仪、X射线衍射仪、扫描电镜和硬度计,研究了热处理和镀液中六方氮化硼BN(h)含量对复合镀层自润滑性能和硬度的影响。结果表明,镀液中BN(h)颗粒浓度变化对镀层中P含量的影响不大;镀层经热处理后,在表面形成体心立方Ni 3P,增大了表面硬度,有利于发挥BN(h)的润滑作用,从而有效减小镀层表面的摩擦系数;经热处理的Ni-P-BN(h)-7.5复合镀层属于自润滑性镀层,11500 cm磨损试验中平均摩擦系数仅为0.26,且摩擦系数波动较小。
- Abstract:
- In this paper, chemical co-precipitation and subsequent heat treatment were applied to the surface of Q235 steel to form a Ni-P-BN(h) composite coating. The effects of heat treatment and BN(h) content in the plating solution on the self-lubricating property and hardness of the composite coating were studied by EPMA, XRD, SEM and hardness tester. The results show that the concentration change of BN(h) particles in the plating solution has little effect on the P content in the coating. After heat treatment, Ni3P is formed on the surface of the coating, which increases the surface hardness, promotes BN(h) to play a lubricating role, thereby effectively reduces the friction coefficient of the coating surface. The heat-treated Ni-P-BN(h)-7.5 composite coating belongs to self-lubricating coating, of which the average friction coefficient in 11500 cm wear test is only 0.26, and the friction coefficient fluctuation is relatively small
参考文献/References:
[1] 王迎春, 马壮, 吕广庶, 等. 化学镀Ni-P合金的耐磨性研究[J]. 材料工程, 2000, 53(8): 25-27.
Wang Y C, Ma Z, Lv G S, et al. Study on wearing resistance of electroless Ni-P alloy[J]. Journal of Materials Engineering, 2000, 53(8): 25-27 (in Chinese).
[2] Crobu M, Scorciapino A, Elsener B, et al. The corrosion resistance of electroless deposited nano-crystalline Ni-P alloys[J]. Electrochimica Acta, 2008, 53(8): 3364-3370.
[3] Huang H C, Chung S T, Pan S J, et al. Microstructure evolution and hardening mechanisms of Ni-P electrodeposits[J]. Surface and Coatings Technology, 2010, 205: 2097-2103.
[4] Balaraju J N, Selvi V E, Grips V W, et al. Electrochemical studies on electroless ternary and quaternary Ni-P based alloys[J]. Electrochimica Acta, 2007, 52(3): 1064-1074.
[5] Gawne D T, Ma U. Structure and wear of electroless nickel coatings[J]. Materials Science and Technology, 1987, 3(3): 228-238.
[6] 李富军, 叶涛, 刘定富, 等. 稳定剂对化学镀Ni-P-TiO2复合镀层性能的影响[J]. 电镀与环保, 2019, 39(4): 37-39.
Li F J, Ye T, Liu D F, et al. Effect of stabilizers on properties of electroless Ni-P-TiO2 composite coatings[J]. Electroplating & Pollution Control, 2019, 39(4): 37-39 (in Chinese).
[7] 曾宪光, 陈亚超, 彭静,等. 镍磷氮化硅复合化学镀工艺优化[J]. 电镀与涂饰, 2020, 39(12): 741-743.
Zeng X G, Chen Y C, Peng J, et al. Optimization for electroless plating of nickel-phosphate-silicon nitride composite coating[J]. Electroplating & Finishing, 2020, 39(12): 741-743 (in Chinese).
[8] Ankita S, Singh A. Corrosion and wear study of Ni-P-PTFE-Al2O3 coating: the effect of heat treatment[J]. Central European Journal of Engineering, 2014, 4(1): 80-89.
[9] 苏琪, 刘军松, 刘定富, 等. 热处理对锌-镍-磷-纳米二氧化硅复合电镀层性能的影响[J]. 电镀与涂饰, 2019, 38(23): 1271-1274.
Su Q, Liu J S, Liu D F, et al. Effect of heat treatment on properties of electroplated zinc-nickel-phosphorus-nano-silica composite coating[J]. Electroplating & Finishing, 2019, 38(23): 1271-1274 (in Chinese).
[10] 刘守法, 周兆锋. 第二相增强金属基复合材料研究进展[J]. 热加工工艺, 2018(4): 14-16.
Liu S F, Zhou Z F. Research progress on secondary phase-reinforced metal matrix composite[J]. Hot Working Technology, 2018(4): 14-16 (in Chinese).
[11] Heshmati M, Seifzadeh D, Shoghi P, et al. Duplex Ni-Zn-Cu-P/Ni-P electroless coating on magnesium alloy via maleic acid pretreatment[J]. Surface & Coatings Technology, 2017, 328: 20-29.
[12] Chen W W, Gao W, He Y D. A novel electroless plating of Ni-P-TiO2 nano-composite coatings[J]. Surface & Coatings Technology, 2010, 204(15): 2493-2498.
[13] Voevodin A A, O’Neill J P, Zabinski J S. Nanocomposite tribological coatings for aerospace applications[J]. Surface & Coatings Technology, 1999, 116-119: 36-45.
[14] Voevodin A A, Bultman J and Zabinski J S. Investigation into three-dimensional laser processing of tribological coatings[J]. Surface & Coatings Technology, 1998, 107(1): 12-19.
[15] Gholizadeh-Gheshlaghi M, Seifzadeh D, Shoghi P, et al. Electroless Ni-P/nano-WO3 coating and its mechanical and corrosion protection properties[J]. Journal of Alloys and Compounds, 2018, 769: 149-160.
[16] Farzaneh A, Mohammadi M and Ehteshamzadeh M. Electrochemical and structural properties of electroless Ni-P-SiC nanocomposite coatings[J]. Applied Surface Science, 2013, 276: 697-704.
[17] Ma C Y, Wu F F, Ning Y F, et al. Effect of heat treatment on structures and corrosion characteristics of electroless Ni-P-SiC nanocomposite coatings[J]. Ceramics International, 2014, 40(7): 9279-9284.
[18] Franco M, Sha W, Aldic G, et al. Effect of reinforcement and heat treatment on elevated temperature sliding of electroless Ni-P/SiC composite coatings[J]. Tribology International, 2016, 97: 265-271.
[19] 翟永杰, 乔世杰, 陆小龙, 等. 热处理对激光熔覆γ-(Ni, Fe)/CrB/hBN自润滑耐磨复合涂层力学性能的影响[J]. 材料热处理学报. 2015, 36(12): 229-235.
Zhai Y J, Qiao S J, Lu X L, et al. Effects of heat treatment on mechanical properties of γ-(Ni, Fe)/CrB/hBN self-lubrication anti-wear composite coatings by laser cladding[J]. Transactions of Materials and Heat Treatment, 2015, 36(12): 229-235 (in Chinese).
[20] Hou K H, Hwu W H, Ke S T, et al. Ni-P-SiC composite produced by pulse and direct current plating[J]. Materials Chemistry and Physics, 2006, 100: 54-59.
备注/Memo
收稿日期: 2021-03-27 修回日期: 2021-05-04 通信作者: 赵金国(1972-),男,山西太原人,硕士,副教授,高级工程师,主要研究方向:汽车机械及车身结构材料研究,email:zhaojinguo1974@qq.com。